Skip to content
Brass CNC Parts

Brass reference / Leaded brass

CW617N CuZn40Pb2

The standard European brass for hot stamped and machined fittings and valve bodies, the EU counterpart of C377.

Also known as CuZn40Pb2, European hot stamping brass, MS58, CZ122. Published typical values for the alloy, never a promise from a shop.

80Machinability, C360 = 100
1.6 to 2.5%Lead, over the 0.25% line
PoorDezincification resistance
360 to 480 MPaTypical tensile strength

Composition

ElementNominal weight %
Copper57.0 to 59.0
Lead1.6 to 2.5
Aluminium0.05 max
Iron0.3 max
Nickel0.3 max
Tin0.3 max
Zincremainder

Properties

  • UNSC37700 (nearest)
  • EN equivalentCuZn40Pb2 / CW617N
  • DIN2.0402 CuZn40Pb2
  • JISC3771
  • BSCZ122
  • Hardness60 to 80 HRB
  • Density8.44 g/cm3
  • Typical tolerance±0.05 mm as stamped, tighter where machined
  • Common formsRod, bar and hot stamping billet

What it is for, and what it is not

Specify it for

  • Hot stamped valve bodies and fittings made in Europe
  • Parts that are forged then machined on the sealing features
  • European drawings that call for CuZn40Pb2 or MS58
  • Gas and heating fittings outside potable water

Do not specify it for

  • US wetted potable water parts, it is far over the NSF/ANSI 372 lead limit
  • EU drinking water fittings after the 4MS lead limits, use CW511L or CW724R
  • Hot water where dezincification is a risk, use CW602N

What a buyer should know

If a European drawing says CuZn40Pb2, MS58 or CZ122 it means this alloy, and it is the European counterpart of C377 forging brass with near identical composition. It is the default for hot stamping because the alpha-beta structure flows well at forging temperature and the lead keeps the machining fast afterwards. It does not pass the EU drinking water lead limits that came in through the 4MS common approach, so European water fittings are moving to CW511L and CW724R. Composition note: the 2024 edition of EN 12165 changed the composition of CW617N (Table 8 in the DIN list of changes). The limits on this page may predate that edition, so use the standard and the mill certificate for limits.

Nominal lead is 1.6 to 2.5 percent, which is above the 0.25 percent weighted average limit that NSF/ANSI 372 sets for wetted potable water surfaces. See NSF/ANSI 61 and 372 and RoHS exemption 6(c).

Dezincification resistance is poor, so this alloy is the wrong choice sitting in hot water or seawater regardless of how well it machines. See dezincification and the grades that resist it.

Closest alternatives

AlloyLead %Mach.DZRWhy you might switch
C377 forging brassC377001.5 to 2.580PoorHot forged to a near net shape then machined only where a sealing face or thread requires it.
C69300 silicon brassC69300under 0.0980HighThe usual lead-free answer for potable water, roughly twice as strong as C360 and highly dezincification resistant.
Bismuth brassC49300 / C49350under 0.2580ModerateBismuth replaces lead as the chip breaker, so it behaves closest to C360 on an existing C360 program.

All 16 alloys compared · Cross reference

Need a shop that runs CW617N?

Send the drawing. We reply within 24 business hours with one itemised quote for the finished parts.

Get a quote