Brass reference / Tin brass
C443 admiralty brass
A 70/30 brass with tin and arsenic for condenser tubes, highly dezincification resistant and slow to cut.
Also known as Admiralty brass, Arsenical admiralty, Alloy 443, Inhibited admiralty. Published typical values for the alloy, never a promise from a shop.
Composition
| Element | Nominal weight % |
|---|---|
| Copper | 70.0 to 73.0 |
| Tin | 0.9 to 1.2 |
| Arsenic | 0.02 to 0.06 |
| Lead | 0.07 max |
| Zinc | remainder |
Properties
- UNSC44300
- EN equivalentCuZn28Sn1As / CW706R
- DIN2.0470 CuZn28Sn1
- JISC4430
- BSCZ111
- Hardness40 to 60 HRB annealed
- Density8.53 g/cm3
- Typical tolerance±0.05 mm on tube wall, tighter where machined
- Common formsTube, some sheet and strip
What it is for, and what it is not
Specify it for
- Condenser, evaporator and heat exchanger tubes
- Ferrules and tube fittings in fresh and brackish water
- Distiller tubes
Do not specify it for
- Turned parts from bar, it is rated 30 and rarely stocked as bar
- Seawater at high velocity, where aluminium brass or a copper nickel does better
- Anything where C464 naval brass is stocked and would serve
What a buyer should know
Cartridge brass with 1 percent tin and a trace of arsenic. The arsenic inhibits dezincification and the tin helps in water, which made this the condenser tube alloy of the steam age. It arrives as tube, and machined parts from it are ferrules and fittings cut from that tube. For a turned bar part in a corrosive environment, naval brass is the more available choice.
Closest alternatives
| Alloy | Lead % | Mach. | DZR | Why you might switch |
|---|---|---|---|---|
| C464 naval brassC46400 | under 0.20 | 30 | High | About 1 percent tin added for seawater and dezincification resistance, at a heavy cost in machinability. |
| C260 cartridge brassC26000 | trace | 30 | Poor | Made for deep drawing and cold forming, not for cutting, and rated 30 against C360 at 100. |
| C230 red brassC23000 | under 0.05 | 30 | High | A high copper brass that does not dezincify, supplied mostly as tube and pipe, and slow to machine. |
Need a shop that runs C443?
Send the drawing. We reply within 24 business hours with one itemised quote for the finished parts.