Free-cutting brass C360 turns with carbide at published starting speeds of roughly 200 to 400 m/min (650 to 1,300 sfm) and feeds of 0.1 to 0.4 mm/rev, usually dry or with light coolant. Lead-free grades such as C69300 start 20 to 40 percent slower with sharp positive rake tools and chip control. Confirm every figure with the tool maker.
Free-cutting brass C360 is the fastest metal most shops ever cut. Published starting points for carbide turning sit around 200 to 400 m/min, feeds of 0.1 to 0.4 mm/rev, usually dry, with tool life measured in thousands of parts. Every figure here is a published typical starting value for the alloy, not a promise from any shop, and the tool maker’s chart wins if it disagrees.
Lead-free brass is where the numbers move. Silicon brass C69300 and bismuth brass both rate 80 against C360 at 100, and a shop starts them 20 to 40 percent slower, with sharp positive rake tools and attention to chip control. That gap is not a detail. On a bar-fed lathe, cycle time is the price of the part.
Why brass runs so fast
The lead in C360, nominally 2.5 to 3.7 percent, does not dissolve in the copper and zinc. It sits as soft particles through the structure. When a tool passes, each particle is a weak point that snaps the chip into short pieces, and the lead itself smears across the tool face as a lubricant.
Short chips clear the tool without wrapping. Low cutting force means no deflection and no chatter. Little heat goes into the tool, so a polished carbide insert runs for a shift without a visible wear land. Built-up edge, the layer of workpiece that welds to a tool face in gummy metals, hardly forms in leaded brass.
That is why C360 is the 100 mark on the machinability scale and the alloy to assume unless a rule forbids it.
Starting points for C360
| Operation | Speed, carbide unless noted | Feed | Notes |
|---|---|---|---|
| Turning, roughing | 200 to 400 m/min (650 to 1,300 sfm) | 0.2 to 0.4 mm/rev | Uncoated, polished, positive rake insert |
| Turning, finishing | 250 to 450 m/min (800 to 1,500 sfm) | 0.05 to 0.15 mm/rev | Nose radius sets the finish |
| Drilling, solid carbide | 100 to 200 m/min (330 to 650 sfm) | 0.05 to 0.25 mm/rev by diameter | Through coolant helps on deep holes |
| Drilling, HSS | 50 to 90 m/min (160 to 300 sfm) | 0.05 to 0.25 mm/rev | Dub the lips to zero rake on breakthrough |
| Tapping, HSS cut tap | 15 to 30 m/min (50 to 100 sfm) | Feed equals pitch | Form taps run faster, see the tap maker |
| Milling, solid carbide end mill | 150 to 300 m/min (500 to 1,000 sfm) | 0.03 to 0.12 mm per tooth | Two or three flutes for chip room |
| Reaming | 20 to 50 m/min (65 to 160 sfm) | 0.1 to 0.3 mm/rev | Slow speed, firm feed |
Published typical values for free-cutting brass with modern tooling, compiled from tool maker guidance and the Copper Development Association datasheet for C36000. They describe the alloy, not a promise from any shop. Confirm each figure with the tool maker’s chart for the specific tool.
Two things stop a shop reaching the top of those ranges. The first is spindle speed. Surface speed is set by diameter, as the Wikipedia page on speeds and feeds shows, so a 6 mm pin at 300 m/min needs about 16,000 rpm and many lathes stop short of that. On small Swiss parts the spindle caps the speed, not the alloy. The second is rigidity. An old lathe with worn ways chatters long before the insert complains.
What lead-free brass changes
Take the lead out and the chip no longer breaks itself.
Silicon brass C69300 replaces the lead with about 3 percent silicon. The silicon forms hard phases that break the chip a little and give the alloy roughly twice the strength of C360, so cutting forces rise and the chip comes off as a curl rather than a short needle. The hard phases are abrasive, so tool wear rises too. Bismuth brass, the C49300 family, keeps a chip-breaking particle in the structure and behaves closest to C360. Both rate 80 on the scale, and the Copper Development Association datasheet for C69300 carries the same figure.
Four adjustments follow from that.
Speed comes down. Start at 60 to 80 percent of the C360 figure. Full C360 speed is possible on a rigid machine, but insert life drops sharply and the finish suffers.
Rake goes positive and the edge stays sharp. A zero rake insert that works in C360 pushes lead-free brass rather than shearing it, leaving a rubbed surface, a hot chip and a built-up edge that tears the finish. Sharp, polished, positive rake geometry solves most of it.
Chip control becomes a job. Long curled chips wrap a guide bush or pack a drill flute. Chip breaker geometry, a peck cycle on deep holes and higher pressure coolant all help. A shop that has never run lead-free brass learns this on the first bar.
Built-up edge shows up at low speed. Lead-free brass welds to the tool at slow surface speeds in a way C360 does not. The cure is to run a little faster, keep the edge sharp and keep the coolant on.
The full choice between the alloys is in leaded and lead-free brass compared. For machining, treat lead-free brass as a different metal that happens to be yellow.
Need a quote for this part? Get a quote for your brass parts
Rake angle: the old rule and the new one
Anyone who learned to drill brass on a manual machine was taught to stone the lips to zero rake. A twist drill has a positive rake at the outer lip, and in soft brass that edge grabs on breakthrough, pulls the drill forward and either snaps it or hogs the hole. Dubbing the lips flat stops the grab. Old turning practice went the same way: zero or slightly negative rake so the tool scrapes rather than digs.
Modern carbide tooling has moved the other way. Inserts for non-ferrous work use a sharp, polished, positive rake edge, often uncoated, because a keen edge at high speed leaves the finish straight off the tool. On a CNC lathe with a rigid feed drive there is nothing for the tool to grab, so the old reason for zero rake is gone.
Both practices are still in use and both suit the setup they belong to. What matters to a buyer is that lead-free brass only works well with the modern one. A shop that dubs its drills and runs zero rake inserts makes good C360 parts and poor C69300 parts.
Dry or with coolant
Leaded brass with carbide is often cut dry or with an air blast, because the chip carries the heat away and the finish needs no lubricant. Swiss lathes run in cutting oil regardless, because the guide bush needs it.
Coolant earns its place in three cases. It flushes the flute on deep holes. It keeps the built-up edge down on lead-free brass. And it holds a tight dimension steady on a long run where heat would otherwise drift it.
One caution on water-based coolant. Left on the part it stains brass and can leave a white zinc deposit. Wash and dry the parts promptly whatever the coolant was.
Why this matters to a buyer
A buyer never writes speeds and feeds on a drawing, and should not. The shop owns the process. But the figures explain three things about the quote.
Cycle time is the price. On a bar-fed lathe the hour rate is fixed. A part that runs 40 seconds costs about two thirds of one that runs 60. Every figure in the table above is seconds per feature, multiplied by the quantity.
Lead-free costs more per minute and per tool. The slower speed, the higher insert wear and the chip handling all land in the machining line of the quote before the higher bar price is counted.
A shop’s numbers tell you what it runs. Ask whether it has a lead-free job on the floor now. A shop that answers with speeds and a chip story has done it. A shop that says brass is brass has not.
What to put on the RFQ
Not speeds. Give the shop what it needs to pick them.
Material: C360 (CuZn36Pb3), half hard bar.
Or: lead-free, NSF/ANSI 372 compliant alloy, C69300 or equivalent.
Quantity: 2,000 now, repeating quarterly.
Tightest tolerance: bore 6.00 H7. Surface finish Ra 0.8 on sealing face.
Threads: 1/4-18 NPT, gauge required.
The alloy sets the speed. The tolerance and finish set the feed. The quantity decides whether a shop tunes the process or runs a safe default. With those on the page the quote reflects real cycle time.
Ready to see what your part actually costs to run? Send the drawing and say which alloy, or which rule, decides it. We quote the finished parts within 24 business hours and place the work with one of the partner shops that turn brass.
Frequently asked questions
What speed should I run C360 brass at with carbide?
Published starting points for turning C360 with an uncoated carbide insert sit around 200 to 400 m/min, which is 650 to 1,300 sfm, at 0.1 to 0.4 mm/rev depending on whether the pass is roughing or finishing. On small diameters the spindle runs out of rpm before the insert runs out of speed. Treat the figures as a starting point and confirm them with the insert maker's chart.
How much slower does lead-free brass machine?
As a starting point, 20 to 40 percent slower than C360, with the same feed band. Silicon brass C69300 and bismuth brass both carry a published machinability rating of 80 against C360 at 100. The rating understates the difference in practice, because the longer chip and the higher tool wear cost time beyond the raw speed reduction. Sharp positive rake tooling recovers some of it.
Should brass be machined dry or with coolant?
Leaded brass with carbide is often cut dry or with an air blast, and the finish does not suffer. Coolant earns its place on deep holes, on lead-free brass where it suppresses built-up edge and on long runs where thermal growth would drift a tight dimension. Swiss lathes run in oil either way. Whatever is used, wash and dry the parts afterwards, because coolant residue stains brass.
Why were drills for brass ground to zero rake?
A standard twist drill has a positive rake at the lip, and in soft brass that keen edge grabs on breakthrough, pulling the drill into the hole. Flattening the lips, called dubbing, stops the grab on manual and older machines. On a rigid CNC feed drive the grab cannot happen, and modern polished carbide tooling for brass uses positive rake for a better finish. Both practices are still current.
Alloys in this guide
| Alloy | Lead % | Mach. | DZR |
|---|---|---|---|
| C360 free-cutting brassC36000 · CuZn36Pb3 / CW603N | 2.5 to 3.7 | 100 | Poor |
| C69300 silicon brassC69300 · CuZn21Si3P / CW724R | under 0.09 | 80 | High |
Published typical values for the alloy. Machinability against C360 at 100. Not a promise from a shop.
Sources
- Copper Development Association, C36000 alloy datasheet alloys.copper.org
- Copper Development Association, C69300 alloy datasheet alloys.copper.org
- Wikipedia, Speeds and feeds en.wikipedia.org
Need a quote for this part?
Send the drawing. We read it, send one itemised quote for the finished parts within 24 business hours and place the work with a partner shop that turns brass. Brass only.
Get a quote for your brass parts