Published September 27, 2026. Reviewed for the facts in the corrections log.
A roll tap forms the thread by displacing brass without cutting a chip. It needs a larger drill, gives a smoother and stronger thread and suits blind holes and ductile lead-free brass. A cut tap removes material, tolerates a wider drill band and is the default on C360. Specify thread class and gauge, not the tap, unless forming is unacceptable.
A roll tap, also called a form tap, makes the thread by pushing brass into shape. No chip is cut. A cut tap shears the thread out and leaves a chip behind. In brass, both work, and the difference lands in three places: the drill size, the thread’s surface and strength, and what the shop can do in a blind hole.
For a buyer the practical answer is short. Specify the thread class and the gauge, say whether a formed thread is acceptable and leave the tap choice to the shop. The one exception is a thread where the minor diameter does a job, because a formed thread has a split crest there and a cut thread does not.
How each one makes the thread
A cut tap is a hardened screw with flutes ground into it. Each flute edge takes a small chip as the tap advances, and the chips have to go somewhere. In a through hole they push ahead. In a blind hole they pack in the bottom or wind back up the flutes, which is where taps break.
A roll tap has no flutes. Its cross section is a polygon with rounded lobes, and each lobe presses into the wall and displaces metal into the thread form. The metal that would have been a chip flows up to form the crest. Nothing is removed, so there is nothing to clear, and the solid section resists breakage far better than a fluted one.
Because the crest is formed by metal flowing in from two sides, it meets in the middle with a small groove at the minor diameter. Tap makers call it a split crest. It is normal, it passes a go and no-go gauge and it is the most common reason an inspector who has not seen a formed thread rejects a good part.
The drill size difference
This is the part that catches people. A roll tap displaces metal inward to form the crest, so the hole starts larger. Drill too small and the torque climbs, the crest over fills and the tap can seize. Drill too large and the thread is shallow.
| Thread | Cut tap drill | Roll tap drill | Difference |
|---|---|---|---|
| M3 x 0.5 | 2.5 mm | 2.8 mm | 0.3 mm |
| M4 x 0.7 | 3.3 mm | 3.7 mm | 0.4 mm |
| M5 x 0.8 | 4.2 mm | 4.6 mm | 0.4 mm |
| M6 x 1.0 | 5.0 mm | 5.5 mm | 0.5 mm |
| M8 x 1.25 | 6.8 mm | 7.4 mm | 0.6 mm |
| M10 x 1.5 | 8.5 mm | 9.3 mm | 0.8 mm |
| 1/4-20 UNC | 5.1 mm (#7) | 5.8 mm | 0.7 mm |
| 3/8-16 UNC | 7.9 mm (5/16) | 8.8 mm | 0.9 mm |
Published typical values from tap maker charts for roughly 65 to 75 percent thread. Confirm with the chart for the specific tap. The roll tap drill also carries a tighter tolerance, commonly plus or minus 0.03 to 0.05 mm, because it sets the minor diameter directly.
That tolerance is the hidden cost. A cut tap forgives a drill that wandered a little. A roll tap does not, so the shop reams or checks the drill diameter more often.
Thread strength and surface
In a ductile metal a formed thread is stronger than a cut one. The grain flows around the profile instead of being cut across, the flank is burnished smooth and there is no tool mark to start a crack. Pull-out strength and fatigue life both rise, and the smoother flank gives a more consistent torque.
In brass the gain is real but smaller than in steel or aluminium, because brass is already easy to thread cleanly and free-cutting brass has soft lead particles through it that interrupt the flow. The larger benefit in brass is the chip, not the strength.
Where each one is right in brass
Cut tap, the default on C360. Free-cutting brass cuts a short chip that clears itself. Cut taps are cheap, run at published speeds around 15 to 30 m/min in brass and tolerate a loose drill size. On a through hole in C360 there is rarely a reason to do anything else.
Roll tap, when the hole is blind, small or near a bore. No chips means nothing packed in the bottom of a blind hole and nothing fouling a cross hole that breaks into the bore. Under about M6 the breakage argument is strong, since a roll tap is a solid section. Chips in a cross drilled passage are the same problem described in deburring brass parts and cross holes.
Roll tap, on lead-free brass. This is the interesting case. Silicon brass C69300 is more ductile than C360 and has no lead particles to break the flow, so it forms very cleanly. It is also stronger, so tap torque is higher and the tap holder must handle it. Bismuth brass is less ductile and forms less predictably, so the shop should trial it. Cut tapping works too, but the long chip that lead-free brass throws is harder to clear from a small blind hole, which pushes the choice toward forming.
Cut tap, where the minor diameter matters. If the thread also acts as a pilot bore, seals on its minor diameter or feeds a gas or hydraulic system where the crest fold could trap contamination, specify a cut thread and say why.
Need a quote for this part? Get a quote for your brass parts
Gauging is the same either way
Both thread types are inspected with go and no-go plug gauges to the class on the drawing. For metric threads that is ISO 1502 and a class such as 6H. For unified threads it is ASME B1.2 and a class such as 2B or 3B. The gauge checks pitch diameter, and it does not care how the thread was made.
Two things to watch. A roll tap in a thin wall can push the outside diameter out by a few hundredths, so gauge the outside of a thin boss as well as the thread. And a roll tap run with too small a drill over fills the crest, which can foul the go gauge and shows up as a tight thread rather than an out of tolerance one.
For sealing pipe threads, NPT and BSPT, the tapered form is cut, not rolled, and the gauge is a taper plug checked by hand tight engagement. That is a different subject, covered in NPT and BSP threads on brass fittings.
The lathe alternatives
Not every thread in brass is tapped. On a lathe, two other routes exist and a good shop picks between all three.
Single point threading uses a turning tool and a synchronised feed to cut the thread one pass at a time. It handles any pitch and diameter, gives full control of the pitch diameter and is the usual route for external threads and for internal threads above about M12. It needs a runout groove at the end of the thread, which is worth drawing in. The tool forms are described on the Wikipedia page on taps and dies.
Thread milling uses a rotating cutter on a helical path. One tool covers every diameter of a given pitch, the class is adjusted by offset, a blind hole gets nearly full depth and a broken cutter does not lodge in the part. It is slower per hole than tapping and more common on milled brass blocks than on turned parts.
The shop chooses. What it needs from you is the class, the depth of full thread and any relief.
What to put on the drawing
The thread callout does most of the work. Add the three things a callout does not carry.
M6x1 - 6H, 4 places. Full thread 9 min, drill depth 12 max.
Formed (roll tapped) threads acceptable.
Verify with go and no-go plug gauges to ISO 1502.
Or, where the crest matters:
1/4-20 UNC-2B, 2 places. Full thread 8 min.
Cut threads only, minor diameter is a pilot fit.
Gauge to ASME B1.2.
State the class. State the full thread depth and the drill depth separately, because a roll tap needs no extra drill depth for chips but a cut tap in a blind hole does. State whether forming is acceptable. If you say nothing, most shops form small blind threads in brass and cut the rest, which is usually right.
Have a threaded brass part to quote? Send the drawing with the thread classes marked. We quote the finished parts within 24 business hours and place the work with one of the partner shops that thread brass every day.
Frequently asked questions
Is a roll tapped thread weaker than a cut thread?
No. In a ductile metal a formed thread is usually stronger, because the grain flows around the profile instead of being cut across and the flank is burnished smooth. In brass the gain is smaller than in steel, since brass threads cleanly by either method. The visible difference is the split crest at the minor diameter, which is normal on a formed thread and passes the same gauges.
Why does a roll tap need a bigger drill?
Because it removes nothing. The metal that forms the crest has to come from the wall of the hole, so the hole starts larger than it would for a cut tap, typically by 0.3 to 0.9 mm across the common sizes. The drill also carries a tighter tolerance, since it sets the minor diameter directly. Too small a hole raises the torque and can seize the tap.
Can lead-free brass be roll tapped?
Yes, and often better than leaded brass. Silicon brass C69300 is ductile and has no lead particles to interrupt the flow, so it forms a clean thread, although its higher strength raises the tap torque. Bismuth brass is less ductile and should be trialled first. Cut tapping also works, but the long chip that lead-free brass produces is harder to clear from a small blind hole.
Do I need to tell the shop which tap to use?
Usually not. Give the thread class, the full thread depth, the drill depth for a blind hole and the gauge requirement. Say whether a formed thread is acceptable. A shop will then form small blind threads in brass and cut the rest. Only specify cut threads when the minor diameter does a job, such as a pilot fit or a passage where a crest fold could trap contamination.
Sources
- ASME B1.2, Gages and Gaging for Unified Inch Screw Threads asme.org
- Wikipedia, Tap and die en.wikipedia.org
Need a quote for this part?
Send the drawing. We read it, send one itemised quote for the finished parts within 24 business hours and place the work with a partner shop that turns brass. Brass only.
Get a quote for your brass parts