Reference / Brass density chart
Brass Density Chart by Alloy: g/cm3 and lb/in3
Machined brass runs from 8.30 g/cm3 for lead-free C69300 to about 8.67 for red brass C23000. Free-cutting C36000 sits at 8.50, or 0.307 lb/in3.
Published typical values, read on the source pages listed under the table on 25 October 2026. They are not a lot certificate and not a promise from a shop.
| Alloy | Designation | Density g/cm3 | Density lb/in3 | Source | Other sources opened |
|---|---|---|---|---|---|
| C23000 red brass, 85 percent | UNS C23000 | 8.67 | 0.313 | A | The same Wieland Concast page prints 0.316 lb/in3 in its machinability table. AmesWeb gives 8.75 g/cm3 (0.316) and EngineeringToolbox 8746 kg/m3. |
| C26000 cartridge brass, 70/30 | UNS C26000 | 8.53 | 0.308 | A | AmesWeb 8.53 g/cm3 (0.308). EngineeringToolbox 8530 kg/m3. |
| C27000 yellow brass, 65 percent | UNS C27000 | 8.47 | 0.306 | B | EngineeringToolbox 8470 kg/m3. |
| C36000 free-cutting brass | UNS C36000, CW603N nearest | 8.50 | 0.307 | C | Fisk Alloy 8.5 g/cm3 and 0.307. E-Z LOK (H) 8.49 g/cm3 and 0.307. AmesWeb 8.50 and 0.307. |
| C38500 free-cutting brass, architectural bronze | UNS C38500 | 8.47 | 0.306 | D | Single source. |
| C46400 naval brass | UNS C46400 | 8.41 | 0.304 | A | Austral Wright Metals 8.41 g/cm3 and 0.304. |
| C69300 lead-free silicon brass | UNS C69300 | 8.30 | 0.300 | A | Single source. The page prints 8.3 g/cm3 and 0.3 lb/in3. |
| C35330 dezincification-resistant machining brass | UNS C35330 | 8.46 | 0.306 c | E | Single source, metric only. |
| CW614N brass, CuZn39Pb3 | EN CW614N, 2.0401 | 8.47 | 0.306 c | F | Single source, metric only. |
| Admiralty brass, generic | No UNS given by the source | 8.53 | 0.308 c | G | Source prints 8525 kg/m3. |
Source letters refer to the list below. c The page gives g/cm3 only; lb/in3 is computed at 1 lb/in3 = 27.68 g/cm3 (453.59237 g per lb and 2.54 cm per inch). 1 g/cm3 equals 1000 kg/m3. Temperature basis is 20 C (68 F) where the source states it.
Sources
- A. Wieland Concast, C26000, C46400, C23000 and C69300 product pages, "physical properties provided by CDA"
- B. AmesWeb, density of copper and copper alloys table
- C. Fisk Alloy, MA36B C36000 free-cutting brass
- D. Austral Wright Metals, free cutting brass alloy 385, UNS C38500
- E. Austral Wright Metals, dezincification resistant machining brass alloy 352, UNS C35330
- F. Bikar, brass CW614N product data page
- G. EngineeringToolbox, densities of metals and alloys
- H. E-Z LOK, brass material properties (C36000)
The Copper Development Association alloy pages could not be opened on the day this chart was compiled, so no figure here is quoted from them directly. The Wieland Concast pages print CDA physical property lines, which is why they are used for the wrought grades they cover. We could not open a datasheet with a readable density for grades such as C37700, CW617N and CW511L, and left them out rather than guess.
How to read the chart
Use the g/cm3 column for drawings in millimetres and the lb/in3 column for drawings in inches. Multiply volume in cm3 by g/cm3 to get grams. A 20 mm round part 50 mm long has a volume of 15.71 cm3, so in C36000 at 8.50 it weighs 133.5 g and in C69300 at 8.30 it weighs 130.4 g, about 2.4 percent less.
The spread between grades is small. From C69300 at 8.30 to C23000 at 8.67 is 4.5 percent, and 5.4 percent if you take the 8.75 that two other tables print for red brass. Swapping C36000 for C69300 changes the piece weight by about 2 percent.
Where two sources differ, the table shows the one read on the most direct page and lists the others. The red brass row is the clearest case. One Wieland Concast page prints 0.313 lb/in3 in its physical property block and 0.316 in its machinability table. Alloys are cast to composition ranges and sources round differently, so treat the third decimal as approximate.
Three mistakes show up in weight estimates. The first is using the density of copper, 8.96 g/cm3 on the AmesWeb page, for brass; it overstates the weight by about 5 percent. The second is mixing kg/m3 with g/cm3: 8500 kg/m3 is 8.5 g/cm3. The third is applying a bar density to a cast or sintered part, which can be lower because of porosity.
On an RFQ, name the alloy by UNS or EN number and say which density basis a weight limit uses. If part weight is a requirement, write it as a weight with a tolerance and ask the shop to weigh a first article rather than calculate it. For bar consumption and material cost at your price, use the bar weight calculator. To choose the alloy first, read the brass grades guide, and for the forms the bar comes in see brass bar stock sizes and forms.
Questions about brass density
What density should I use for brass in a weight estimate?
Use the density of the alloy on the drawing, not a single figure for all brass. Free-cutting C36000 is about 8.50 g/cm3, naval brass C46400 about 8.41 and lead-free C69300 about 8.30. Across the grades in this chart the spread is under 5 percent, so a generic 8.5 is close for a quote estimate. Weigh a sample if a weight limit is a requirement.
Why do two sources give different densities for the same brass?
Alloys are made to composition ranges, not one recipe, so the zinc, lead and tin content moves the density a little. Sources also round differently and some print a wrought value and some a typical value across tempers. The red brass row shows it: one mill page prints 0.313 lb/in3 in one table and 0.316 in another. Treat the third digit as approximate.
Are these figures a promise from a shop?
No. They are published typical values for the alloy, read on the pages named under the table. A supplier certificate or your own weighing of the delivered bar is what proves a lot. We place your RFQ with partner shops that turn brass, and they use the material they stock, so confirm the grade and density basis in the quote.
Have the grade and the drawing? Get it quoted.
Send the drawing. We reply within 24 business hours with one itemised quote for the finished parts.