Hot shortness is cracking during hot working caused by a liquid phase at the grain boundaries. In brass that phase is lead, which melts at 327 degrees Celsius and is liquid at any forging temperature. Free-cutting brass C360 carries 2.5 to 3.7 percent lead and tears in the die. C377 forging brass carries 1.5 to 2.5 percent and forges well.
Free-cutting brass C360 is the easiest metal to machine and a poor choice for a forging die, and the reason is the same 3 percent of lead that breaks the chip. Lead melts at 327 degrees Celsius. At forging temperature it is a liquid sitting between the grains, and a metal with liquid between its grains tears the moment you stretch it. That tearing is called hot shortness.
C377 forging brass exists to solve it. Less lead, so the liquid film at the boundaries is thinner and broken up, and a copper-zinc balance that turns mostly into the plastic beta phase at forging heat. It fills a die cleanly and still machines at 80 against C360 at 100.
What hot shortness is
Hot shortness is a loss of ductility at hot working temperature, caused by a phase that is liquid at that temperature wetting the grain boundaries. The grains themselves are fine. The joints between them are not, because a liquid film cannot carry a tensile load.
Under compression the boundaries are held shut and nothing happens. Under tension they open along the film and the crack runs between the grains rather than through them. The fracture is intergranular, granular to the eye and often carries a grey sheen of the metal that caused it.
This is why the same alloy behaves so differently in two hot processes. C360 bar is made by hot extrusion at the mill, and extrusion holds the billet in compression on every side inside the container. The boundaries never see tension, so the lead film does no harm. A forging die is different. The metal flows outward into the impression and into the flash gutter, and the free surface and the flash zone are in tension. That is where the tears start.
Two dials: lead and zinc
Zinc dissolves in copper. Lead does not, at any temperature the alloy sees. In C360 the 2.5 to 3.7 percent lead sits as discrete particles at the grain boundaries and inside the grains, and every one of those particles is molten well before the billet reaches the die. The more lead, the more continuous the liquid film along the boundaries.
The second dial is the structure. Brass with more than about 35 percent zinc carries some beta phase at room temperature, and on heating the beta fraction grows. Beta is body-centred cubic and far more plastic at hot working temperature than alpha, so a brass that is mostly beta at forging heat flows around obstacles instead of tearing at them. A single phase alpha brass such as C260 has no beta to flow, which is why it cold forms rather than hot forges.
C377 sits where both dials point the right way. Copper 58 to 61 percent, so a high beta fraction at forging heat, and lead 1.5 to 2.5 percent, low enough that the film is discontinuous. C385 architectural brass carries as much lead as C360 but even less copper, and its larger beta fraction is what lets it forge into door and window hardware. C360 has the most lead and the least beta of the three. That is the wrong corner.
| Grade | Copper, nominal % | Lead, nominal % | Machinability | Die forging |
|---|---|---|---|---|
| C377 forging brass | 58 to 61 | 1.5 to 2.5 | 80 | The forging grade |
| C385 architectural | 55 to 59 | 2.5 to 3.5 | 90 | Forges, high beta fraction carries the lead |
| C360 free-cutting | 60 to 63 | 2.5 to 3.7 | 100 | Tears at the flash, extruded to bar instead |
| C69300 silicon brass | 73 to 77 | under 0.09 | 80 | Forges, lead-free, thinner supply |
| C260 cartridge | 68.5 to 71.5 | trace | 30 | Single phase alpha, cold formed not forged |
Published typical values for the alloy. They describe the material, not a promise from any shop. Machinability is rated against C360 at 100.
The forging window
The Copper Development Association lists a hot working range for C377 of roughly 650 to 760 degrees Celsius, and shops run toward the top of that band so the billet is still plastic when it reaches the die.
Both ends of the window bite.
Too cold and the beta fraction drops, the flow stress climbs, the die does not fill and the metal cracks from low ductility rather than from the lead. The forging looks underfilled at the corners and ribs.
Too hot and zinc begins to burn off the surface, the grains coarsen, the lead film is more mobile and hot shortness gets worse. Zinc boils at 907 degrees Celsius, so the top of the window is set by the zinc rather than the copper.
Time at temperature matters as much as the number. A billet soaked too long coarsens the grain and lets the lead migrate toward the boundaries. This is the shop’s problem to manage. The buyer’s part of it is to specify an alloy that has a window at all.
Need a quote for this part? Get a quote for your brass parts
What it looks like on a part
Hot shortness cracks show up in the die or at trim, not in service.
- Along the flash line, where the metal was pulled outward into the gutter under tension.
- Radial cracks on the rim of a flange or across the corners of a hex, where the metal stretched furthest.
- On the outside of an upset section, where a bulge put the surface in tension.
- Rough, granular fracture faces that follow the grain boundaries rather than cutting across them, sometimes with a grey sheen of lead.
A shop that forges brass sees these at trim and scraps the part. The one to watch for is the small tear that gets machined over. It sits under a sealing face, passes visual inspection and opens on the pressure test. That is one reason forged pressure fittings are pressure tested after machining rather than only inspected.
Not the same crack as stress corrosion
Both are intergranular, which is why they get confused, and they have nothing else in common.
Hot shortness happens in the die at forging temperature. It is driven by liquid lead and it is visible before the part is machined. Stress corrosion cracking happens at room temperature, weeks or months after assembly. It is driven by residual tensile stress plus ammonia. Its sensitivity comes from zinc content, not lead.
There is one overlap worth knowing. A forging pushed at the cold end of the window carries more residual stress into service, and a forging that is cold worked afterwards, staked, crimped or thread rolled, needs the same stress relief at 330 to 350 degrees Celsius as a bar turned part would. Surviving the die does not make a part immune to the second crack.
Alloy for the process, not for the lathe
The mistake that causes most of this is inherited material. A part designed to be turned from C360 bar gets redrawn for forging when the volume justifies a die, and the material callout comes along unchanged. The shop either quotes C377 and hopes nobody objects, or forges C360 and scraps a third of the run.
Specify the alloy for the process the part will go through. Turned from bar, C360. Forged then machined, C377, its European equivalent CW612N or a forging brass to the same specification. Leave the exact grade open so the shop can use the stock it holds. If the part is a potable water component the forging grade is lead-free, and C69300 forges well but is held by fewer stockists.
The volume arithmetic that decides whether to forge at all is covered in forging or machining a brass part. The alloy question in this post only arises once that arithmetic says forge.
What to put on the drawing
Hot forged from C377 (C37700, CW612N) or
equivalent forging brass. Forgings free of laps,
tears and flash line cracks. Pressure test after
machining, see note 6.
State the process and name a forging grade with an “or equivalent”. Put the pressure test on the drawing so the tear that got machined over is found in the shop rather than in the field.
The two alloys are compared side by side in C360 vs C377 brass.
Have a bulky brass part heading for a die? Send the drawing with the annual quantity and say it is to be forged. We place it with a partner shop that already forges brass rather than one that would be learning on your part.
Frequently asked questions
What is hot shortness in brass?
A loss of ductility at hot working temperature caused by a liquid phase sitting between the grains. In brass the liquid is lead, which melts at 327 degrees Celsius and is fully molten long before the metal reaches forging heat. Under tension the grain boundaries open along the liquid film and the part tears. The crack is intergranular and appears during forging, not in service.
Can C360 free-cutting brass be hot forged at all?
It is done, with narrow temperature control and simple shapes, but it is not the grade to choose for a forging. C360 carries 2.5 to 3.7 percent lead and has less of the plastic beta phase at forging heat than C377, so it tears at the flash and on free surfaces. C360 is hot extruded into bar at the mill because extrusion holds the metal in compression, which is a different loading from a die.
Is hot shortness the same as stress corrosion cracking?
No, though both cracks run between the grains. Hot shortness happens in the die at forging temperature and is driven by liquid lead. Stress corrosion cracking happens at room temperature weeks or months after assembly, driven by residual tensile stress and ammonia. The sensitivity comes from zinc rather than lead. A forging that survived the die can still crack in service if it is cold worked afterwards and not stress relieved.
Do lead-free brasses have hot shortness?
Much less from lead, since C69300 silicon brass carries under 0.09 percent and forges well, which is why it is used for forged potable water fittings. Bismuth is another low melting element that can wet grain boundaries, so bismuth brasses need more care in hot working. Ask the shop before assuming they forge. Supply of lead-free forging stock is thinner than C377, so check availability before the drawing is fixed.
Alloys in this guide
| Alloy | Lead % | Mach. | DZR |
|---|---|---|---|
| C377 forging brassC37700 · CuZn39Pb2 / CW612N | 1.5 to 2.5 | 80 | Poor |
| C360 free-cutting brassC36000 · CuZn36Pb3 / CW603N | 2.5 to 3.7 | 100 | Poor |
Published typical values for the alloy. Machinability against C360 at 100. Not a promise from a shop.
Sources
- Copper Development Association, C37700 forging brass properties copper.org
- Wikipedia, Lead en.wikipedia.org
Need a quote for this part?
Send the drawing. We read it, send one itemised quote for the finished parts within 24 business hours and place the work with a partner shop that turns brass. Brass only.
Get a quote for your brass parts