Skip to content
Brass CNC Parts

Guides / Process

Cutting O-Ring Grooves in Brass: Depth, Width, Finish and Burr Control

Published November 21, 2026. Reviewed for the facts in the corrections log.

Black nitrile rubber O-rings of the kind that seat in an O-ring groove in brass parts
Photo: R. Henrik Nilsson, CC BY 4.0, via Wikimedia Commons

An O-ring groove in brass is sized from the cord diameter. A static seal usually squeezes the cord 15 to 30 percent, which sets the depth, and the width is about 1.3 to 1.5 times the cord. The groove needs a fine finish, no burrs, and a lead-in chamfer where the O-ring is assembled over an edge.

An O-ring is the cheapest seal in a brass fitting and the one most often blamed when a fitting leaks. In most cases the O-ring is fine and the groove it sits in is not. A groove that is a few tenths of a millimetre off in depth, or has a burr on one edge, will leak at a pressure the design should hold.

This post sets out how to size a groove from the cord diameter, what finish and edge condition it needs, and how to write the callout so a shop cuts it right the first time.

Diagram: O-Ring Grooves in Brass: Dimensions, Finish and Burrs

How an O-ring seals

The O-ring is a round elastomer cord closed into a loop. It sits in a groove, and the mating part presses it so that it squeezes between the groove bottom and that part. The squeeze gives the first seal. System pressure then pushes the cord toward the low-pressure side of the groove, which tightens the seal further. If the groove is too shallow the cord is crushed and will take a permanent set. If it is too deep the cord is barely touched and leaks at low pressure.

So three numbers matter: how much the cord squeezes, how much room it has to spread, and how smooth the surfaces are.

Sizing from the cord diameter

Cord diameter is also called cross-section, CS. Standard cross-sections in inch sizes under AS568 are 0.070, 0.103, 0.139, 0.210 and 0.275 inch, which is 1.78, 2.62, 3.53, 5.33 and 6.99 mm. Metric cords under ISO 3601 are commonly 1.8, 2.65, 3.55, 5.3 and 7.0 mm. Pick the cord first, then cut the groove to the maker’s handbook.

The usual design targets for a static seal in a rigid metal body such as brass:

Item Static seal Dynamic seal
Squeeze on the cord 15 to 30 percent 10 to 20 percent
Gland depth (as a share of the cord) 70 to 85 percent 80 to 90 percent
Groove width (as a multiple of the cord) 1.3 to 1.5 1.3 to 1.5
Gland fill, cord volume over groove volume Under 85 percent Under 85 percent
Groove bottom corner radius About 0.2 to 0.4 mm About 0.2 to 0.4 mm

Published typical design values. The O-ring maker’s handbook and the elastomer data take precedence, and the numbers change with pressure, temperature and fluid.

A worked example. Take a 2.62 mm cord in a static face seal with 20 percent squeeze. Gland depth is 80 percent of 2.62 mm, about 2.10 mm. Groove width at 1.4 times the cord is about 3.7 mm. The cord is squeezed by 0.52 mm and has room to spread sideways, with gland fill near 70 percent so there is still space for thermal growth or swell in the fluid.

Fill matters because rubber does not compress. It changes shape. If the groove is too small for the cord’s volume, the rubber has nowhere to go, pressure builds and the seal extrudes into the gap or tears. The 85 percent limit gives room for swell.

Tolerances

The depth tolerance matters most, because it sets the squeeze. On a 2.62 mm cord, a depth held at plus or minus 0.05 mm gives a squeeze range of about 18 to 22 percent, which is acceptable. A depth held at plus or minus 0.15 mm gives a range of 14 to 26 percent. That may still seal, but the margin is gone. Brass turns and mills to these limits easily on a grooving tool, but a note on the drawing keeps the tolerance from being relaxed. General tolerance ranges and the cost of tighter ones appear in brass machining tolerances and surface finish.

For the groove width the tolerance can be looser, since the cord has room to spread. A tolerance of plus 0.2 mm and minus 0 on a face seal is common.

Surface finish and lay

Finish has two parts: the value and the direction.

The value. Static sealing surfaces on brass are typically Ra 0.8 micrometre or better, with the groove bottom and walls around Ra 1.6 micrometre. Gas and vacuum service ask for finer surfaces than liquid service because gases pass through smaller scratches. Brass turns to these values without a second operation when the tool is sharp and the feed is moderate. Surface roughness explains Ra for readers who need a refresher.

The direction. A turned surface has a lay, a spiral of tool marks. If the lay runs across the seal, the marks form tiny channels from the high-pressure side to the low-pressure side. Even a fine finish will leak if the spiral crosses the seal. On a face groove cut by a grooving tool, the lay is circular, which is correct. On a bore where an O-ring slides, a spiral lay can pump fluid past the seal. For a dynamic bore, specify a ground or burnished finish with the lay running along the seal path, and say so.

Need a quote for this part? Get a quote for your brass parts

Burrs, edges and assembly damage

Brass cuts clean but it still burrs at the groove edges, and a burr is a knife to a rubber seal. The groove edges need to be broken, typically with a radius or a chamfer of 0.1 to 0.3 mm, and free of burrs under a 10x loupe. Deburring cross holes in brass deals with the places where burrs hide.

The other hazard is assembly. When an O-ring slides over a thread, a cross hole or a sharp shoulder on the way into its groove, it can be cut. A lead-in chamfer, usually 15 to 20 degrees and long enough to run the cord up gradually, protects it. Threads, ports and cross holes located under the path of the O-ring should be chamfered or moved. This is a drawing item, not something a shop adds on its own.

Handling matters as well. Brass is soft. A groove face that is dropped into a tote with other parts picks up dents. Tumbling can peen edges and leave media in the groove. Tumbling and vibratory finishing covers the steps to take. Specify packing that keeps the sealing faces apart.

Plating

If the part is plated, the layer thickens the groove walls and shrinks the groove. A 10 micron coating takes 20 microns off the width and 10 microns off the depth, which is small against the usual tolerances, but it also changes the finish. Plating can build up on a sharp corner. Break the edge before plating, and say whether the groove is masked. See brass surface finishes and plating.

Testing the seal

A groove is proven when the assembly passes its leak test, not when the drawing is signed. See leak and pressure testing brass valve bodies for how that test is written.

What to put on the drawing

O-ring groove for 2.62 mm cord, static face seal.
Groove depth 2.10 +/- 0.05. Groove width 3.7 +0.2/-0.
Groove bottom radius 0.3 max. Edges broken 0.1 to 0.3, free of burrs.
Surface finish Ra 1.6 on groove walls and bottom, Ra 0.8 on the sealing face.
Lay circumferential. No tool marks across the sealing face.

Checklist

  • Cord diameter and seal type (static or dynamic) written.
  • Depth, width and tolerance written, not left to a general tolerance.
  • Groove finish and lay direction specified.
  • Edge break and burr limit stated.
  • Lead-in chamfer shown where the O-ring is assembled over an edge.
  • Plating and masking stated.
  • Packing that keeps sealing faces from touching.

Need a brass part with an O-ring groove quoted? Send the drawing. We quote the finished parts within 24 business hours and place the work with one of the partner shops that turn brass.

Frequently asked questions

How deep should an O-ring groove be?

Depth follows from the squeeze you want. For a static seal with 20 percent squeeze the gland depth is about 80 percent of the cord diameter. A 2.62 mm cord gives a gland of about 2.1 mm. Dynamic seals use less squeeze, typically 10 to 20 percent, so the gland is deeper. The O-ring maker's handbook gives the exact table for each cord size.

What surface finish does an O-ring groove need in brass?

The sealing surface that the O-ring presses on should be fine, typically Ra 0.8 micrometre or better for liquids and gases, with groove bottom and walls around Ra 1.6. Brass turns to these finishes without trouble. Check the handbook of the O-ring maker for the exact values, since dynamic seals ask for more.

Why does a groove leak even when the dimensions are right?

Usually because of a burr, a scratch across the sealing face or a spiral tool mark running across the seal. A spiral lay can form a leak path along the lay line. Specify circumferential lay on a static groove face, and ask for the groove edges to be broken and free of burrs.

Alloys in this guide

AlloyLead %Mach.DZR
C360 free-cutting brassC36000 · CuZn36Pb3 / CW603N2.5 to 3.7100Poor
C69300 silicon brassC69300 · CuZn21Si3P / CW724Runder 0.0980High

Published typical values for the alloy. Machinability against C360 at 100. Not a promise from a shop.

Sources

  1. Wikipedia, O-ring en.wikipedia.org
  2. Wikipedia, Surface roughness en.wikipedia.org

Need a quote for this part?

Send the drawing. We read it, send one itemised quote for the finished parts within 24 business hours and place the work with a partner shop that turns brass. Brass only.

Get a quote for your brass parts

Keep reading

Get a quote